Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of RAVAMID® B GF40 NC - PA6-GF40 - Ravago Group

Material Data Center offers the following functions for RAVAMID® B GF40 NC:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Ravamid B datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Product Texts
Resistant. Negligible, reversible or no changes in mass and dimensions.

Please consider the information about the application of the materials.
Processing/Physical CharacteristicsValueUnitTest Standard
ISO Data
Molding shrinkage, parallel 0.2 % ISO 294-4, 2577
Molding shrinkage, normal 0.8 % ISO 294-4, 2577
Mechanical propertiesValueUnitTest Standard
ISO Data
Tensile Modulus 10300 MPa ISO 527
Stress at break 170 MPa ISO 527
Strain at break 2.5 % ISO 527
Flexural modulus, 23°C 9300 MPa ISO 178
Charpy impact strength, +23°C 65 kJ/m² ISO 179/1eU
Charpy notched impact strength, +23°C 10.5 kJ/m² ISO 179/1eA
Izod notched impact strength, +23°C 11 kJ/m² ISO 180/1A
Thermal propertiesValueUnitTest Standard
ISO Data
Temp. of deflection under load, 1.80 MPa 215 °C ISO 75-1/-2
Vicat softening temperature, B 225 °C ISO 306
Burning behav. at 1.5 mm nom. thickn. HB class IEC 60695-11-10
Thickness tested 1.6 mm -
Burning behav. at thickness h HB class IEC 60695-11-10
Thickness tested 3.2 mm -
Burning rate, FMVSS, Thickness 1 mm 100 mm/min ISO 3795 (FMVSS 302)
Glow Wire Flammability Index (GWFI) 650 °C IEC 60695-2-12
GWFI - thickness tested (1) 2 mm -
Other propertiesValueUnitTest Standard
Humidity absorption 0.15 % Sim. to ISO 62
Density 1450 kg/m³ ISO 1183
Processing Recommendation Injection MoldingValueUnitTest Standard
Pre-drying - Temperature 75 °C -
Pre-drying - Time 3 - 4 h -
Processing humidity ≤0.12 % -
Melt temperature 240 - 270 °C -
Mold temperature 70 - 90 °C -
Zone 1 220 - 230 °C -
Zone 2 230 - 245 °C -
Zone 3 250 - 260 °C -
Nozzle temperature 250 - 260 °C -
Screw speed 50 - 80 rpm -
Back pressure 0.4 - 0.8 MPa -
Holding pressure 6 - 8 MPa -
Characteristics
Processing
Injection Molding
Delivery form
Natural Color
Special Characteristics
U.V. stabilized or stable to weather, Heat stabilized or stable to heat
Certifications
Recycled Resin Content
Regional Availability
Europe
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.